<cite id="1l9pj"><span id="1l9pj"><var id="1l9pj"></var></span></cite><span id="1l9pj"><dl id="1l9pj"></dl></span>
<ruby id="1l9pj"><i id="1l9pj"></i></ruby>
<span id="1l9pj"><dl id="1l9pj"><ruby id="1l9pj"></ruby></dl></span><span id="1l9pj"></span><ruby id="1l9pj"><dl id="1l9pj"><ruby id="1l9pj"></ruby></dl></ruby>
<span id="1l9pj"></span>
<ruby id="1l9pj"></ruby>
<strike id="1l9pj"></strike>
<span id="1l9pj"></span>
<strike id="1l9pj"><i id="1l9pj"><cite id="1l9pj"></cite></i></strike>
<strike id="1l9pj"></strike>
<ruby id="1l9pj"><dl id="1l9pj"><del id="1l9pj"></del></dl></ruby>
<strike id="1l9pj"></strike>
<strike id="1l9pj"></strike><strike id="1l9pj"><dl id="1l9pj"><del id="1l9pj"></del></dl></strike>
<span id="1l9pj"><video id="1l9pj"><ruby id="1l9pj"></ruby></video></span>
<strike id="1l9pj"></strike>
<span id="1l9pj"><dl id="1l9pj"></dl></span>

涂料施工常見問題及應急處理辦法

導讀:
本文介紹在涂料施工過程中常遇見的幾類問題及應急處理辦法。

1、垂流:在垂直面涂裝時,涂膜向下流呈,凸部的現象,涂裝效果不佳。

產生原因:可能一次涂裝過厚或涮涂料濃度過高,噴槍氣過大,出漆量過多,噴嘴離涂裝特過近。

處理方法:稀釋過當粘度,調整噴槍氣,壓力3.5-4.5kg/m2,壓適當及出量,距離適宜(15cm-20cm)。

2、刷痕:涂刷后,涂膜呈條狀凹凸不平的現象。

產生原因:施工時,粘度過高,濕膜再涂。

處理方法:將涂料調至適當粘度,再涂時,底膜需基本干燥,刷子用力不要過大。

3、針孔:涂膜干燥后,涂面呈現小孔狀,該小孔由基材于表面的現象。

產生原因:涂膜施噴太厚,干燥溫度過高,被涂物有濕氣,塵漆等。

處理方法:一次施噴厚度不得太厚,控制適當的干燥溫度,保持被涂物無污塵等。

4、干噴現象:涂料噴涂時經霧化的涂料未到被涂物以前即已干燥一部分,再附著時形成粗糙的涂面。

產生原因:噴涂時噴槍口與被涂物距離過遠,噴槍氣壓過高等原因造成。

處理方法:調整噴槍口與被涂物距離,約15cm-20cm,壓力調整為3.5-4.5kg/m2

5、白化現象:涂膜表面蒼白,無預期光澤。

產生原因:濕度過高(80%以上),稀釋劑菡發過快,被涂物太冷。

處理方法:涂裝濕度應80%以上,或可加5-10%的防白水,要用過快干的稀釋劑,被涂物不要太冷。

6、剝離脫落:涂膜從被涂物表面成片掉下。

產生原因:基材有蠟、油、水等,下涂未干而再涂,底材過于平滑,墻面已粉化或采用低劣補土,附著力不夠。

處理方法:將底材徹底除干凈,確保無蠟、油、水等雜物,已粉化的舊墻必須鏟除干凈;用油性批土,或水性批土批平,完全干燥后再涂膜。

7、桔皮現象:涂膜不平滑,象桔皮狀凹凸涂膜。

產生原因:稀釋劑蒸發太快,噴壓力不定或壓力過大,吹附距離太遠,一次噴涂太厚,底層未干再涂。

處理方法:使用適當的稀釋液,控制噴槍壓力,距離要適中,不要一次厚涂,底層完全干燥再涂。

8、褪色現象:涂膜數日后,顏色部分褪掉,色澤不均一。

產生原因:新增未完全干燥,堿性太重,造成色澤退掉。

處理方法:新墻應一個月后涂裝,用環氧底漆對底。